- WPS: the instructions. PQR: the proof the instructions work. WPQ: the proof each welder can follow them.
- Current codes: AWS D1.1/D1.1M:2025, the 25th edition, and the 2025 edition of ASME Section IX.
- Change an essential variable beyond its limits and you need a new procedure qualification test.
- A welder who does not use a process for 6 months loses that qualification.
- A weld map ties every weld on a drawing to its WPS, the welder and the inspection result.
Welding procedure specification, PQR and WPQ at a glance
Three documents work together, and each code has its own rules for them. The table gives each one's definition and the code or source it comes from.
| Document | Definition | Code or source |
|---|---|---|
| Welding procedure specification (WPS) | "A document providing the required welding variables for a specific application to assure repeatability by properly trained welders and welding operators" | AWS A3.0, quoted by FHWA |
| Procedure qualification record (PQR) | "A record of welding variables used to produce an acceptable test weldment and the results of tests conducted on the weldment" | AWS A3.0, quoted by FHWA |
| Welder performance qualification (WPQ) | "The demonstration of a welder's or welding operator's ability to produce" acceptable welds | LANL welding standard GWS 1-05 |
| Prequalified WPS | "A written welding procedure with the ranges taken from a set of pre-qualified variables as defined in the AWS codes" | LANL welding glossary |
| Weld map | Drawings with sketches and tables that tie design, weld plan, shop drawings, welder identification and NDE together | DoD UFGS 33 01 50.75 |
Code editions: AWS released "D1.1/D1.1M:2025, Structural Welding Code - Steel" on April 17, 2025 (AWS); it is the 25th edition, with an amendment dated January 12, 2026 (AWS, PDF). ASME lists Section IX editions as "2025, 2023, 2021" (ASME). Sources for the table: FHWA, PDF, LANL GWS 1-05, PDF, LANL glossary, PDF and UFGS, PDF.
What goes on a WPS? A welding procedure specification template
ASME publishes a suggested layout, Form QW-482, whose sections follow the variables of Section IX (ASME Form QW-482, PDF). The template below uses those sections. The example column is invented, shows the kind of entry each field needs, and is not a qualified procedure: a real WPS takes its ranges from its supporting PQRs or from the prequalified limits of the code.
| Section (QW-482) | What to record | Example entry (invented) |
|---|---|---|
| Header | WPS number, revision, date, supporting PQR numbers, process and type | WPS-117 rev 2; PQR-117; FCAW, semi-automatic |
| Joints (QW-402) | Joint design, groove details, backing, root spacing, sketch | Fillet and single-V groove; steel backing |
| Base metals (QW-403) | P-No. and Group No. joined, thickness range qualified | P-No. 1 Group 1 to P-No. 1 Group 1 |
| Filler metals (QW-404) | SFA specification, AWS classification, F-No., A-No., size | SFA-5.20, E71T-1C, F-No. 6, A-No. 1, 1.2 mm |
| Positions (QW-405) | Positions of groove and fillet, progression | All positions; vertical up |
| Preheat (QW-406) | Minimum preheat, maximum interpass temperature | Code minimum for the thickness; interpass limit stated |
| Postweld heat treatment (QW-407) | Temperature and time range, or none | None |
| Gas (QW-408) | Shielding gas, mixture and flow rate | 100% CO2 |
| Electrical characteristics (QW-409) | Current and polarity; amps and volts for each electrode size, position and thickness; travel speed | DCEP; amperage, voltage and travel speed ranges from the PQR |
| Technique (QW-410) | Stringer or weave, cleaning, single or multiple pass, contact tube distance | Stringer beads; wire brush between passes |
The form itself says "amps and volts, or power or energy range, should be recorded for each electrode size, position, and thickness, etc." and lists base metals by "P-No." and "Group No." and filler metals by "Spec. No. (SFA)", "AWS No. (Class)", "F-No." and "A-No." (ASME Form QW-482, PDF). ISO has its own content rule: ISO 15609-1 "specifies requirements for the content of welding procedure specifications for arc welding processes" (ISO 15609-1:2019 preview, PDF).
Prequalified WPS vs qualified by test: when do you need a PQR?
Under AWS D1.1, clause 5 "contains the requirements for exempting a Welding Procedure Specification (WPS) from the WPS qualification requirements of this code", and clause 6 covers "WPS qualification and the performance qualification tests required to be passed by all welding personnel" (AWS D1.1:2025 preview, PDF). A prequalified WPS works only if every variable stays inside the prequalified limits: the joint, the process, the steel and filler combination and the other conditions the clause sets. Step outside any of them and the procedure needs a PQR.
Other codes are stricter. The bridge welding code is a clear case: "only SMAW procedures in conformance with clause 1.3.2, and for fracture-critical welding clause 12.7.1, may be used without testing" (FHWA, PDF). ASME Section IX qualifies procedures by test, and its suggested PQR form is headed "Record Actual Variables Used to Weld Test Coupon" (ASME Form QW-483, PDF). The PQR is a record of what happened on the test day; the WPS is the range you are allowed to work within because of it.
What are essential, supplementary essential and nonessential variables?
Each code sorts the variables on a WPS by how much they affect the weld. Essential variables affect mechanical properties: "if the WPS is changed outside of prescribed limits for these essential variables, a new qualification test must be performed based on the change" (FHWA, PDF). Under ASME Section IX, supplementary essential variables are added "when impact toughness is required", in the words of ASME's own Section IX course description, for example on pressure equipment that must meet impact tests. Nonessential variables, such as many technique details, can be changed by revising the WPS without a new test.
Typical essential variables include a change of base metal group, a change of filler metal group, adding or removing postweld heat treatment, and a change of process. The exact list depends on the process and the code, so read the variable tables for your process before revising a WPS, and record which PQR supports each range.
How does welder qualification (WPQ) work, and when does it lapse?
A WPQ records that a named welder made an acceptable test weld under a WPS; ASME's suggested form is QW-484A (ASME Form QW-484A, PDF). The qualification covers ranges of position, thickness and filler metal, and it lapses if it is not used. LANL's standard puts it plainly: "When a welder has not welded with a process during a period of 6 months or more, the welder's qualifications for that process shall expire" (LANL GWS 1-05, PDF). Alberta's pressure equipment regulator points to the same "6 month continuity requirement" in ASME Section IX paragraph QW-322 (ABSA, PDF).
FHWA notes that the six-month period "is not based on a study of welder skill loss over time" (FHWA, PDF), but it is the rule, and auditors check it. Keep a continuity log: each welder, each process, and the date and job of the last weld made with it.
What is a weld map, and what should it show?
A weld map gives every weld on a job an identity. The Department of Defense guide specification defines it as "drawing(s) containing sketches and tables which correlate design, weld plan, shop drawings, welder identification, and nondestructive examination (NDE)" (UFGS 33 01 50.75, PDF). In practice it is a marked-up drawing with a number on each joint and a table like the one below. Rows are invented.
| Weld ID | Joint and location | WPS | Welder ID | Date | Inspection and result | Repair |
|---|---|---|---|---|---|---|
| W-01 | Base plate to column, fillet, all around | WPS-117 | W-23 | 12 Nov | Visual: accept | None |
| W-02 | Column splice, complete joint penetration groove | WPS-121 | W-23 | 12 Nov | UT: reject, lack of fusion | R1, WPS-121, retested UT accept |
| W-03 | Stiffener to web, fillet | WPS-117 | W-41 | 13 Nov | Visual: accept; MT: accept | None |
When a weld is rejected, the repair is a new row tied to the same weld ID, and the nonconformance belongs in the NCR log. A weld map kept this way answers the questions a customer, an inspector or a court asks later: who welded this joint, to which procedure, and how was it checked.
AWS D1.1 vs ASME Section IX vs ISO 15614: which code applies?
The contract or the governing code decides. AWS D1.1 covers structural steel; ASME Section IX qualifies procedures and welders for work under the ASME boiler, pressure vessel and piping codes; and the ISO route uses ISO 15609-1 for the WPS and ISO 15614-1, which "specifies how a preliminary welding procedure specification is qualified by welding procedure tests" (ISO 15614-1:2017 preview, PDF). ISO 15614-1 has two levels, and "level 1 is based on requirements of ASME Section IX and level 2 is based on the previous issues of this document", which helps when one procedure must satisfy customers on both sides of the Atlantic.
Common WPS and welding record mistakes
Audit findings on welding usually come from the paperwork, not the welds:
- A WPS whose ranges are wider than its supporting PQR allows.
- A "prequalified" WPS that uses a joint, filler or process outside the prequalified limits.
- No supporting PQR number on the WPS, or a PQR that cannot be found.
- Welder continuity not tracked, so lapsed qualifications are discovered at audit.
- WPSs at the welding station that are a revision behind the controlled copy.
- Weld maps that stop at the drawing and never record the welder or the inspection result.
Can your company get paid by AI companies for its welding procedures and weld records?
Your company can get paid for these records. Research on AI for welding keeps running into the same limit: little real data. A machine learning system that recommends welding procedures, and can "directly generate the welding procedure specification required by the enterprise format", was built from a dataset with "492 samples" (Intelligence and Robotics, 2023). Researchers predicting weld quality write that "deep learning offers the potential to identify the relationships in available process data and predict the weld quality" (arXiv 2310.12632), and a 2025 study of multimodal language models on welding stresses "the importance of fine-tuning, domain-specific data" (arXiv 2503.16537).
AI data buyers publish payouts of $100K to $5M for established companies' records, and most ask for 30 or more staff. A fabricator's library of WPSs and PQRs with their test results, welder records and weld maps linked to inspection outcomes is the domain data those studies lack. Our guide to licensing manufacturing quality records to AI companies covers what buyers ask for and what customer drawings and terms keep out. Shops with skilled welders can also look at programs that pay to record manufacturing work.
We help you license your data. Origin Data Partners is an independent data partner that helps business owners value and license their company records: the company pays Origin nothing, and a buyer may pay Origin when a deal completes. Describe the records first: how many WPSs and PQRs, which codes, how many years of weld maps and inspection records, and which jobs were for customers whose drawings must stay out. Then see what your company's records could be worth. Not the owner? Advisers can introduce the company.
How we checked this
We read every source on this page on 21 November 2026: the American Welding Society's release notice and its D1.1:2025 preview, ASME's Section IX edition list, course page and suggested forms QW-482, QW-483 and QW-484A, FHWA's bridge welding guidance, Los Alamos National Laboratory's welding standards, a Department of Defense guide specification, Alberta's pressure equipment regulator, the ISO 15609-1 and 15614-1 previews, and the research papers cited.
What we could not verify: the full text of AWS D1.1:2025 and of ASME Section IX, which are sold, so code wording is quoted from the codes' own previews and forms and from government documents that cite them. We could not read the exact 2025 wording of QW-322, so the six-month rule is quoted from LANL's standard and Alberta's bulletin. The example entries are invented.
Common questions
What is the difference between a WPS and a PQR?
The WPS is the instruction: the ranges of variables a welder works within on production welds. The PQR is the evidence: a record of the actual variables used to weld a test coupon and the results of the tests on it. A qualified WPS lists the PQRs that support it, and its ranges cannot go beyond what those PQRs and the code allow.
What is a prequalified WPS in AWS D1.1?
It is a procedure that AWS D1.1 exempts from qualification testing because every variable stays within limits the code has already proven: specific joints, processes, steels, filler metals and other conditions in clause 5. If any variable falls outside those limits, the procedure must be qualified by test under clause 6 with a PQR. Other codes, such as the bridge code, allow far less.
How long is a welder qualification valid?
Under ASME Section IX and most structural codes, a welder stays qualified for a process as long as they keep using it: if they do not weld with that process for 6 months or more, the qualification for it expires and they must retest. Many companies also require periodic retesting. Track the date of each welder's last weld by process in a continuity log.
What are essential variables in a welding procedure?
Essential variables are the WPS variables that affect the mechanical properties of the weld, such as base metal group, filler metal group, postweld heat treatment and process. Changing one beyond its qualified limits requires a new procedure qualification test. Supplementary essential variables apply when impact toughness is required, and nonessential variables can be changed by revising the WPS.
Who writes and signs a welding procedure specification?
The company that does the welding, usually through its welding engineer or welding coordinator, who prepares the WPS from the PQR results. Under the codes, the organization takes responsibility for its procedures and qualifications, and an authorized person certifies the PQR and WPQ records. Customers and inspectors review the WPS but do not own it.
What is a weld map used for?
A weld map gives each weld on a drawing an ID and links it to the WPS used, the welder who made it, the date, and the inspection method and result, including any repair. It lets an inspector, customer or later investigation trace any joint back to its procedure and welder, and it shows at a glance which welds still need inspection.
Can a fabrication shop license its WPS and weld records to AI companies?
Yes, where the records are the shop's own and customer contracts allow it. A library of WPSs and PQRs with test results, welder records and weld maps linked to inspection outcomes is scarce domain data for AI that plans or checks welding. Customer drawings and personal details of welders need care. Start by describing the record set without sharing files.
Sources and further reading
- FHWA: Steel bridge welding guidance, HIF-19-088 (PDF)
- Los Alamos National Laboratory Engineering Standards: welding glossary (PDF)
- Los Alamos National Laboratory: GWS 1-04, welding procedure qualification (PDF)
- Los Alamos National Laboratory: GWS 1-05, welder performance qualification (PDF)
- American Welding Society: release of D1.1/D1.1M:2025
- AWS D1.1/D1.1M:2025 Amendment 1, preview (PDF)
- AWS D1.1/D1.1M:2025, preview (PDF)
- ASME: Boiler and Pressure Vessel Code 2025 editions
- ASME: BPV Code Section IX course (welding, brazing and fusing qualifications)
- ASME Section IX Form QW-482, suggested WPS format (PDF)
- ASME Section IX Form QW-483, suggested PQR format (PDF)
- ASME Section IX Form QW-484A, suggested WPQ format (PDF)
- ABSA (Alberta pressure equipment safety authority): Information Bulletin IB24-013 (PDF)
- Unified Facilities Guide Specifications (DoD), UFGS 33 01 50.75 (PDF)
- ISO 15609-1:2019, specification of welding procedures for arc welding (preview, PDF)
- ISO 15614-1:2017, welding procedure tests for steels and nickel alloys (preview, PDF)
- Intelligence and Robotics (2023): machine learning for welding procedure specifications
- arXiv 2310.12632: deep learning for weld quality prediction from process data
- arXiv 2503.16537: multimodal language models on welding